This article compares the characteristics of UNS C63200 and UNS C95800 copper alloys, detailing their chemical compositions, mechanical properties, performance at different temperatures, industry applications, shape, size, production standards, and additional relevant factors.
Kimyasal bileşim
Öğe
C63200 (%)
C95800 (%)
Alüminyum (Al)
8.7 – 9.5
8,5 – 9,5
Nikel (Ni)
4.0 – 4.8
4.0 – 5.0
Demir (Fe)
3.5 – 4.3
3,5 – 4,5
Manganez (Mn)
1.2 – 2.0
00,8 – 1,5
Silikon (Si)
0.1
0.1
Kurşun (Pb)
00,02
00,03
Bakır
Denge
79
Mekanik özellikler
Mülk
C63200
C95800
Sertlik (Rockwell B)
85-95
85-90
Gerilme direnci
550MPa
620 MPa
Akma dayanımı
300 MPa
380 MPa
Kopma Uzaması
8%
Elastik modülü
117 GPa
117 GPa
Charpy Etkisi
25.0 J
15.0 J
İşlenebilirlik
70
40
Farklı Sıcaklıklarda Performans
Mülk
C63200
C95800
Erime noktası
1033°C (1911°F)
1060°C (1940°F)
Termal iletkenlik
50.0 W/mK (346 BTU in/hr.ft²°F)
40.0 W/mK (276 BTU in/hr.ft²°F)
Termal Genleşme Katsayısı
16.3 µm/m°C
16,5 mikron/m°C
Endüstri Uygulamaları
Başvuru
C63200
C95800
Denizcilik Bileşenleri
Evet
Evet
Pump and Valve Components
Evet
Evet
Electrical Connectors
Sınırlı
Sınırlı
Heavy Machinery Parts
Sınırlı
Evet
Şekil ve boyut
Attribute
C63200
C95800
Available Shapes
Rods, Bars
Rods, Bars
Standard Sizes
Various
Various
Common Forms
Sheet, Plate
Sheet, Plate
Üretim Standartları
Standart
C63200
C95800
ASTM
B505, B150
B505, B150
ASME
SFA 5.7
SFA 5.7
SAE
J461, J463
J461, J463
Kaynak ve İşleme
İşleme Yöntemi
C63200
C95800
Welding Compatibility
Good (with precautions)
Sınırlı
Preferred Welding Method
Gas shielded, resistance
Somewhat difficult
Parlatma
Good polishing capability
Moderate polishing capability
Isı tedavisi
Evet
Evet
Soğuk İşleme
Moderate capacity
Sınırlı
Avantajlar ve dezavantajlar
Attribute
C63200
C95800
Avantajları
Good strength, corrosion resistant
Excellent wear resistance, high strength
Dezavantajları
Lower wear resistance compared to C95800
Higher cost, lower machinability
Benzer Ürünler
Benzer Ürünler
Özellikler
Copper Nickel Alloys
Good corrosion resistance, suitable for marine applications.
Aluminium Bronze Alloys
High strength and corrosion resistance, often used in similar applications.
Benzer Ürünlerin Karşılaştırılması
Ürün
Korozyon Direnci
Kuvvet
Uygulamalar
UNS C63200
Yüksek
Ilıman
Marine, Pumps, Valves
UNS C95800
Daha yüksek
Yüksek
Pumps, Heavy Machinery
Copper Nickel Alloys
Çok Yüksek
Ilıman
Marine, Plumbing
Çözüm
In conclusion, both UNS C63200 and UNS C95800 copper alloys exhibit unique properties that make them suitable for different applications. C63200 is characterized by its good strength and corrosion resistance, making it a reliable option for marine components. In contrast, C95800 provides superior wear resistance and is better suited for high-stress applications, particularly in heavy machinery. Understanding these distinctions will facilitate informed choices in material selection for various engineering requirements. If you have any further questions or need additional information, feel free to ask!
En iyi deneyimleri sağlamak amacıyla, cihaz bilgilerini depolamak ve/veya bunlara erişmek için çerezler gibi teknolojiler kullanıyoruz. Bu teknolojilere izin vermek, bu sitedeki gezinme davranışı veya benzersiz kimlikler gibi verileri işlememize olanak tanıyacaktır. Onay vermemek veya onayı geri çekmek belirli özellikleri ve işlevleri olumsuz etkileyebilir.
Fonksiyonel
Her zaman aktif
Teknik depolama veya erişimin, abone veya kullanıcı tarafından açıkça talep edilen belirli bir hizmetin kullanımının sağlanması meşru amacı veya yalnızca bir elektronik iletişim ağı üzerinden bir iletişimin iletilmesini gerçekleştirmek amacıyla kesinlikle gerekli olması.
Tercihler
Teknik depolama veya erişimin, abone veya kullanıcı tarafından talep edilmeyen tercihlerin saklanmasının meşru amacı için gerekli olması.
İstatistik
Yalnızca istatistiksel amaçlarla kullanılan teknik depolama veya erişim.Yalnızca anonim istatistiksel amaçlarla kullanılan teknik depolama veya erişim. Mahkeme celbi, İnternet Servis Sağlayıcınızın gönüllü uyumu veya üçüncü bir tarafın ek kayıtları olmadan, tek başına bu amaç için saklanan veya alınan bilgiler genellikle kimliğinizi belirlemek için kullanılamaz.
Pazarlama
Teknik depolama veya erişim, reklam göndermek amacıyla kullanıcı profilleri oluşturmak veya kullanıcıyı benzer pazarlama amaçları doğrultusunda bir web sitesinde veya çeşitli web sitelerinde izlemek için gereklidir.